Moisture Barriers for Flexible Electronics

Murugavel Ganesan
by
2
Share Facebook X LinkedIn WhatsApp Email

Defects on plastic substrates such as pinholes, cracks and grain boundaries cause a "pore effect", where oxygen and water molecules are able to seep through the plastic barrier and into the active material. For applications such as flexible OLED displays, organic solar cells, or even electrophoretic displays, sensitivity to oxygen and moisture compromises device lifetime significantly. This means that in order to achieve adequate lifetime for flexible devices that would make viable commercial products, the pathway for oxygen and moisture down into the active layers must be blocked.

Why flexible devices need a barrier at all

A glass display is sealed between two sheets of glass, and glass lets almost no water through. A flexible display or solar cell replaces the glass with plastic film, and plastic is porous to water vapor and oxygen on a molecular scale. The organic materials in an OLED or an organic solar cell react with that water and oxygen, and the device darkens or loses efficiency. So every flexible organic device needs a barrier film on top of, or as part of, its plastic substrate.

The challenge is the level of protection. A barrier good enough for a bag of snacks is about a million times too leaky for an OLED, as the deep dive below shows.

The Tera-Barrier approach (as of 2011)

Tera-Barrier Films is a portfolio company of Exploit Technologies Pte. Ltd. (ETPL), the commercialization arm of Singapore's Agency for Science, Technology and Research (A*STAR), and of Applied Ventures, LLC, the venture capital arm of Applied Materials, Inc., as of August 2009. The company was incubated by Exploit Technologies Pte. Ltd. as a flagship program for two years prior to spin-off.

Current barrier technologies focus on reducing these defects by using alternate organic and inorganic multilayers coated on plastic. In contrast, Tera-Barrier has taken a different approach to resolve the pore effect, literally plugging the defects in the barrier oxide films using nanoparticles. This reduces the number of barrier layers needed in the construction of the barrier film down to two layers in this nanoengineered barrier stack. Tera-Barrier's barrier stack consists of barrier oxide layers and nanoparticulate sealing layers. The nanoparticles used in the barrier film have a dual function: they seal the defects and also actively react with and retain the moisture and oxygen.

The result is a moisture barrier performance of better than 10-6 g/m2/day, which satisfies even the most stringent requirements for flexible organic device substrates. The barrier film also has a lag time of more than 2,300 hours at 60 °C and 90% RH (the time required for moisture to pass through the barrier film under those conditions).

The barrier is not enough on its own: edge sealing

It is also important to point out that the barrier layer on its own is not an adequate way to keep oxygen and moisture away from the active materials. Moisture ingress can also occur from the side of the device if it is not adequately sealed. This leads to specific requirements in water vapor transmission rates for the sealants used in electronic devices.

Two of the main companies developing these types of adhesives are Henkel and DELO; Henkel focused mainly on thermally cured solutions while DELO focused on UV-cured adhesives.

A trade-off becomes apparent when trying to find the right balance of permeation rates and flexibility. The adhesives with the best water vapor transmission performance are more rigid and would compromise the overall flexibility of the final device. This means that in order to manufacture devices of a given flexibility, permeation performance needs to be sacrificed. Hence a lot of research and development effort is focused on systems that give a good balance between permeation performance and flexibility.

The 2011 event

In-depth presentations from Henkel, DELO and Tera-Barrier, as well as work on other materials, manufacturing and novel devices, were scheduled for Printed Electronics/Photovoltaics Europe in Düsseldorf, Germany, on April 5 and 6, 2011. The original event page is gone; an archived copy of the IDTechEx Printed Electronics and Photovoltaics Europe 2011 page remains.

Deep dive: the numbers and details

This part holds the barrier requirements by application, a worked example of how much water gets through, how such low rates are measured, and what happened to Tera-Barrier later. Skip it if the overview is all you need.

How good a barrier has to be

Water vapor transmission rate (WVTR) is the mass of water that passes through one square meter of film per day.

ApplicationTypical WVTR targetSource
Food and pharmaceutical packagingA few g/m2/dayWith, Helmstedt and Prager, Frontiers in Materials, 2020, Introduction
High-barrier films, including organic electronics encapsulationBelow 10-4 g/m2/daySame review
OLEDsAbout 10-6 g/m2/dayScientific Reports, 2016, abstract

So the OLED requirement is about six orders of magnitude tighter than food packaging.

Worked example: water through a small display

Take a flexible display of 10 cm x 10 cm, which is 0.01 m2, over a 10-year life of about 3,650 days:

Water through = WVTR x area x time

Food-grade film,  1 g/m2/day:    1 x 0.01 x 3650      = 36.5 g
High barrier,  1e-4 g/m2/day: 1e-4 x 0.01 x 3650      = 3.65 mg
OLED grade,    1e-6 g/m2/day: 1e-6 x 0.01 x 3650      = 36.5 micrograms

Even the OLED-grade figure lets some water in. That is why devices also use getters or, as in the Tera-Barrier design, particles that react with and hold the water that does get through.

Lag time

Permeation through a film does not start at full rate. Water first has to diffuse through the thickness of the film; the delay before steady flow is the lag time. For a simple film of thickness L and diffusion coefficient D, the classic time-lag result is tlag = L2 / (6D). Layers that react with water, as the nanoparticle layers do, extend the delay beyond this because the water is consumed on the way. The 2020 Frontiers review notes that water-scavenging particles in adhesives or interlayers increase lag time. Tera-Barrier's 2011 figure of more than 2,300 hours at 60 °C and 90% RH is a lag time, not a steady-state rate.

Why pinholes dominate

The same review explains that permeation of gases is dominated by pinholes and cracks at the nanometer to micrometer scale, while for water, diffusion along chemical defects can dominate when pinholes are few. Stacking alternating organic and inorganic layers works because a defect in one inorganic layer rarely lines up with a defect in the next, so water must travel sideways through the organic layer to find the next hole. Plugging the defects directly, as Tera-Barrier did, attacks the same problem with fewer layers.

Measuring 10-6 g/m2/day

Ordinary permeation testers cannot see such small flows. The 2020 review gives typical detection limits:

MethodApproximate detection limit (g/m2/day)
Coulometric sensor5 x 10-5
Calcium mirror test (electrical or optical)About 10-6
Mass spectrometry1.9 x 10-7 to 1 x 10-6

In the calcium test a thin calcium film under the barrier turns into transparent, non-conducting calcium hydroxide as water arrives, so the change in its resistance or transparency measures the water. The review also notes that ultra-barrier measurements can take months to reach steady state. The 2016 Scientific Reports paper states that at that time no reliable results had been reported in the 10-6 range, and describes an improved equal-pressure method to reach it.

What happened next

In January 2014, Asian Scientist reported that Tera-Barrier Films, described as a spin-off of A*STAR's Institute of Materials Research and Engineering, had developed a stretchable plastic film thinner than aluminum foil, using a layer of nanoparticles encapsulated in polymer shells, aimed at the shelf life of food, pharmaceuticals and electronics. The company said its barrier was about ten times better than the transparent oxide barriers then used for food and medicines.

Further reading

Murugavel Ganesan
About the Author
Murugavel Ganesan
Product Director | SerDes · IVN · Edge AI · Compute | Ex Intel · Infineon

A semiconductor product leader working across product architecture, definition, strategy, and silicon and software execution, from concept through volume production. He has worked with teams across Asia, Europe and the USA, including at Intel, Infineon and ArrayComm.

His work covers ASICs, SoCs, FPGAs and chiplets for wireless, wireline, automotive, IoT and AI, including PCIe, CXL and DDR interfaces alongside RF and mixed-signal design.

Share Facebook X LinkedIn WhatsApp Email

Post a Comment

2 Comments

Your comments will be moderated before it appears here.

  1. Congratulations The new blog looks fantastic! Looking forward to figuring out all the tips and tricks with you!

    ReplyDelete
  2. Thank you to tell us so much useful information. So nice sharing. I’m glad to read it.

    ReplyDelete
Post a Comment

#buttons=(Ok, Go it!) #days=(20)

Our website uses cookies to enhance your experience. Learn more
Ok, Go it!